CoorsTek

Home

Contact

Silicon Carbide

Family Overview

Silicon Carbides (SiC) exhibit characteristically high hardness, wear resistance, corrosion resistance, and strength — even at high temperatures. CoorsTek has engineered a variety of silicon carbide processes and compositions which deliver properties and features optimized for specific application requirements including:

Electrical resistivity: Careful manufacturing control can “tune” the volumetric resistivity.

Lubrication: Certain formulations have graphite embedded into the grain structure for lubrication in exchange for slightly lower flexural strength.

High purity: CoorsTek PureSiC® CVD Silicon Carbide uses chemical vapor deposition (CVD) to produce ultra- pure (>99.9995%) ceramic parts and coatings.

Direct Sintered Silicon Carbide

Direct sintered silicon carbide is extremely resistant to chemical corrosion. Combined with a high maximum use temperature and hardness allows for use in both armor and highly corrosive environment applications and semiconductor processing chambers.

CeraSiC®

A silicon carbide material that is ideal for machine parts that require not only high thermal strength, but also abrasion and corrosion resistance.

Reaction Bonded Silicon Carbide

Reaction bonded silicon carbide, sometimes referred to as siliconized silicon carbide, is a silicon metal infiltrated ceramic. The infiltration gives the material a unique combination of mechanical, thermal, and electrical properties which can be tuned to the application.

PureSiC® CVD Silicon Carbide 

Chemical vapor deposition (CVD) silicon carbide resists corrosion in extreme environments while maintaining the high strength and excellent wear properties of silicon carbide. This capability, combined with the exceptional purity of 99.9995%, is helping make the ultra-clean manufacturing used in semiconductor production run faster and more efficiently.

Liquid Phase Sintered Silicon Carbide 

The low porosity microstructure gives liquid phase (LP) sintered silicon carbide its excellent mechanical properties — especially hardness. This makes LP silicon carbide an outstanding material for many different machinery applications.

Ceramic Expertise

CoorsTek formulates its ceramics to maximize their unique material properties. This includes optimizing the grain size through precise grain structure control.

Our experts can utilize different manufacturing controls, like Chemical Vapor Deposition (CVD) or recrystallization, to manufacture the optimal material for the application.

Brochure Downloads

Download the Silicon Carbide Overview Brochure

Download the PureSic® Silicon Carbide: Semiconductor Applications Brochure.

Download the Semiconductor Furnace Components: Silicon Carbide Components Brochure.

Chemical properties iconElectrical properties iconMechanical properties iconThermal properties icon

Sample Applications by Industry:

Aerospace & Defense


Automotive

Semiconductor

Properties Units CeraSiC®-B
Direct Sintered
SC-RB (SC 2)
Reaction Bonded
UltraSiC™ GI
Graphite Direct Sintered
UltraSiC™ LP
Liquid Phase Sintered
PureSiC®
High Resistivity CVD
PureSiC®
Low Resistivity CVD

Flexural Strength, MOR (20 °C)

MPa 450 462 220 620 468 517

Fracture Toughness, KIc

MPa m1/2 3.5 4.0 3.2 6.0 3.5 3.5

Thermal Conductivity (20 °C)

W/m K 170 125 125 80 140 140

Coefficient of Thermal Expansion

1x10-6/°C 4.5 4.3 4.4 4.8 4.6 4.6

Maximum Use Temperature

°C 1500 1000 1600 1000 1600 1600

Dielectric Strength (6.35mm)

ac-kV/mm — — — — — —

Dielectric Loss (tan δ)

1MHz, 25 °C — — — — — —

Volume Resistivity (25°C)

Ω-cm

>104

<103

-105

—

>105 <0.1